Two Tempers, One Marine Alloy
5083 is the workhorse aluminum-magnesium alloy of shipbuilding and offshore engineering. Under EN 573-3 it contains 4.0 to 4.9 percent magnesium, 0.40 to 1.0 percent manganese, 0.05 to 0.25 percent chromium, and small limits for silicon, iron, copper, zinc, and titanium, with the balance aluminum. The magnesium content gives 5083 its high strength without heat treatment, while the manganese and chromium control grain structure. H116 and H321 are both non-heat-treatable strain-hardened tempers developed for marine plate, and both appear in ASTM B928, the specification written for aluminum plate used in marine service.
What H116 and H321 Actually Mean
H116 is a strain-hardened temper produced with a controlled combination of cold working and thermal history so that the final plate resists exfoliation corrosion and intergranular corrosion in seawater. The temper is defined by its production practice rather than by a fixed final anneal, and plate sold as H116 must pass corrosion tests such as the nitric acid mass loss test of ASTM G67. H321 is strain hardened and then stabilized with a low-temperature thermal treatment. Stabilization removes the tendency of the alloy to sensitize during long service, which makes H321 a dependable choice where welded assemblies stay in contact with seawater.
Mechanical Properties Side by Side
For plate in the common 6 to 50 mm range, EN 485-2 specifies the same tensile property class for 5083-H116 and 5083-H321, with a tensile strength of 305 to 385 MPa and a minimum 0.2 percent proof strength of 215 MPa. ASTM B928 lists the same minimum tensile strength and yield strength for both tempers across comparable thicknesses, with typical elongation around 10 to 12 percent depending on gauge. In practice, H321 plate can show slightly higher consistency in yield strength because the stabilizing treatment evens out the microstructure, while H116 plate is valued for its verified corrosion performance. Hardness levels and fatigue behavior are treated as equivalent by most design codes.
Corrosion Resistance and Classification Approval
Both tempers resist general corrosion in marine atmospheres and immersion because the 5083 alloy forms a stable passive oxide film. The difference is in how each temper guards against localized attack. H116 achieves its resistance through strict production control, and buyers of H116 routinely request mill certificates showing the corrosion test results. H321 achieves similar resistance through stabilization, which prevents precipitation of the magnesium-rich phases that cause intergranular corrosion in sensitized material. Classification societies working under IACS requirements accept both tempers for hull construction, and many shipyards list H116 and H321 as alternates on the same drawing.
Can One Replace the Other?
For most marine plate applications, H321 and H116 are interchangeable because the chemistry, strength minimums, and corrosion requirements are the same or equivalent. The practical rule is to check the thickness, the governing specification, and the classification approval before substitution. H116 is the preferred designation when the project specification demands documented corrosion testing, while H321 is a strong choice when welded structures are annealed or stress-relieved as part of fabrication. When a drawing names one temper, substitution to the other should be confirmed with the designer so that traceability and mill documentation remain valid.
Frequently Asked Questions
Q: Are 5083-H116 and 5083-H321 chemically identical?
Yes. Both tempers are made from the same 5083 alloy with the same composition limits; the difference is only in the thermomechanical processing.
Q: Which temper has higher strength?
Neither. EN 485-2 and ASTM B928 specify the same tensile strength and yield strength minimums for both tempers in comparable thicknesses.
Q: Can H321 replace H116 in hull construction?
In most cases yes, because both are approved marine tempers with equivalent properties, but the replacement must be confirmed with the designer and the classification society involved in the project.
Q: Why is H116 associated with corrosion testing?
H116 is produced under a controlled practice designed to guarantee resistance to exfoliation and intergranular corrosion, and it is commonly delivered with ASTM G67 test results on the mill certificate.
Q: What filler metal is used for welding 5083 plate?
ER5183 and ER5356 are the standard filler alloys for 5083, and they are used for both H116 and H321 plate with the same welding parameters.
Q: Does the stabilizing treatment in H321 affect anodizing or painting?
No. The surface behavior of both tempers is identical for anodizing, painting, and other protective finishes.