6061 and 7075 are two widely specified heat-treatable aluminum alloys, but they sit at opposite ends of the strength-versus-workability scale. 6061 is the versatile 6xxx-series generalist; 7075 is the high-strength 7xxx-series specialist built around zinc.
Need stock or a quotation across 6061 and 7075 mill forms? Send your required alloy, temper, form, dimensions, and destination port to GNEE. Our team confirms availability, lead time, and the applicable standard, then returns a quote with the mill test certificate.
What Are 6061 and 7075 Aluminum Alloys
6061 aluminum belongs to the 6xxx series, the aluminum–magnesium–silicon family. Its strength comes mainly from Mg₂Si precipitation hardening. It is valued for a balance of moderate strength, good corrosion resistance, good weldability, and good formability, which makes it the default structural aluminum across many industries.
7075 aluminum belongs to the 7xxx series, the aluminum–zinc–magnesium–copper family. With roughly 5.1–6.1% zinc plus copper, it is one of the highest-strength aluminum alloys available in commercial quantities. Its weakness is workability and corrosion behavior rather than strength: it machines well but forms and welds poorly compared with 6061.
The two are not competitors in most projects - they are chosen for different dominant requirements. Peak strength points to 7075; ease of fabrication, joining, and corrosion performance point to 6061.
Chemical Composition of 6061 and 7075 Aluminum Alloys
The composition difference is already visible from the series: 6061 carries more silicon, while 7075 carries far more zinc and a higher copper addition. Both contain meaningful magnesium. Values below follow ASTM B209 and EN 573-3 typical ranges.
| Element (wt%) | 6061 | 7075 |
|---|---|---|
| Silicon (Si) | 0.40–0.80 | ≤ 0.40 |
| Iron (Fe) | ≤ 0.70 | ≤ 0.50 |
| Copper (Cu) | 0.15–0.40 | 1.2–2.0 |
| Manganese (Mn) | ≤ 0.15 | ≤ 0.30 |
| Magnesium (Mg) | 0.80–1.20 | 2.1–2.9 |
| Chromium (Cr) | 0.04–0.35 | 0.18–0.28 |
| Zinc (Zn) | ≤ 0.25 | 5.1–6.1 |
| Titanium (Ti) | ≤ 0.15 | ≤ 0.20 |
| Aluminum (Al) | Balance | Balance |
Composition shown for wrought mill product; exact limits depend on form and governing standard. MTC governs for any order.

Mechanical Properties of 6061 vs 7075 Aluminum Alloys in the T6 Condition
Both alloys are heat-treatable, so they are compared at the same temper. In the T6 condition the strength gap is large: 7075-T6/T651 reaches about 1.8 times the tensile strength and roughly 1.6 times the shear strength of 6061-T6. The figures below are minimum or typical values per ASTM B209 and are thickness-dependent.
| Property | 6061-T6 | 7075-T6 / T651 |
|---|---|---|
| Tensile strength | 310 MPa (45 ksi) | 572 MPa (83 ksi) |
| Yield strength | 276 MPa (40 ksi) | 503 MPa (73 ksi) |
| Elongation | 12–17% | 7–11% |
| Hardness (Brinell) | ~ 95 HB | ~ 150 HB |
| Shear strength | ~ 207 MPa (30 ksi) | ~ 331 MPa (48 ksi) |
| Density | 2.70 g/cm³ | 2.81 g/cm³ |
Values are typical for plate/sheet up to common thicknesses; bar, rod, and extrusion may differ. Always confirm against the ordered temper and form.
Physical and Thermal Properties of 6061 and 7075 Aluminum Alloys
Beyond strength, the two alloys differ in density, modulus, conductivity, and thermal expansion. These values are indicative typical figures; the mill certificate governs for a specific lot.
| Property | 6061 | 7075 |
|---|---|---|
| Density | 2.70 g/cm³ | 2.81 g/cm³ |
| Melting range | ~ 580–650 °C | ~ 475–635 °C |
| Elastic modulus | ~ 68.9 GPa | ~ 71.7 GPa |
| Thermal conductivity | ~ 167 W/m·K | ~ 130 W/m·K |
| Coefficient of thermal expansion | ~ 23.6 µm/m·°C | ~ 23.2 µm/m·°C |
The higher density of 7075 (2.81 vs 2.70 g/cm³) is worth noting in weight-sensitive designs: a 7075 part is about 4% heavier per unit volume than the same 6061 part, a trade-off against its roughly 80% higher strength.
Standards and Designations for 6061 and 7075 Aluminum Alloys
Both alloys are covered by the Aluminum Association (AA) designation system and cross-referenced to EN, UNS, ASTM, AMS, and GB standards. Mentioning the governing standard on a request avoids ambiguity.
| Reference | 6061 | 7075 |
|---|---|---|
| AA designation | 6061 | 7075 |
| UNS | A96061 | A97075 |
| EN AW | EN AW-6061 (AlMg1SiCu) | EN AW-7075 (AlZn5.5MgCu) |
| ASTM flat-rolled | ASTM B209 | ASTM B209 |
| ASTM extruded | ASTM B221 | ASTM B221 |
| ASTM bar/rod | ASTM B211 | ASTM B211 |
| AMS plate | AMS-QQ-A-250/16 | AMS-QQ-A-250/12 |
| GB/T 3190 | 6061 | 7075 (7A09 is the nearest national grade) |
EN and GB cross-references are indicative; confirm the exact grade and temper with the order specification.
Heat Treatment and Tempers of 6061 and 7075 Aluminum Alloys
Both alloys are supplied in several tempers, and temper choice changes strength, corrosion resistance, and residual stress.
6061-T6 / T651: solution heat-treated and artificially aged; the most common general-purpose temper. T651 adds stress relief by stretching.
6061-T4: solution heat-treated but not artificially aged; softer and more formable, then ages naturally.
7075-T6 / T651: the most common 7075 temper for plate and bar; highest strength but the least stress-corrosion-cracking (SCC) resistance.
7075-T73 / T7351: overaged for substantially improved SCC resistance at some cost in strength (UTS typically 485–500 MPa).
7075-T76 / T7651: overaged to a lesser degree than T73; a middle point between T6 strength and T73 corrosion resistance.
For 7075, selecting T73 or T76 is the standard way to gain corrosion margin in service where SCC is a concern.
Equivalent Grades and Cross-Reference of 6061 and 7075 Aluminum Alloys
| System | 6061 | 7075 |
|---|---|---|
| AA | 6061 | 7075 |
| UNS | A96061 | A97075 |
| EN AW | EN AW-6061 | EN AW-7075 |
| GB/T 3190 | 6061 | 7075 (≈ 7A09) |
Equivalents are drawn from GB/T, ASTM, and EN standards and are indicative; verify against the specific procurement document.
Corrosion Behavior of 6061 and 7075 Aluminum Alloys
Corrosion resistance is where the two alloys diverge most clearly in service.
General / atmospheric: 6061 shows good resistance in most atmospheres. 7075 shows lower general resistance because of its higher copper and zinc content.
Marine: 6061 performs well with appropriate finishing. 7075 is more vulnerable in saltwater and is usually protected by coating or by selecting the T73 temper.
Galvanic: both are aluminum and behave similarly when coupled to other metals; isolate from more noble metals to avoid galvanic corrosion.
Stress-corrosion cracking (SCC): 6061 has low SCC susceptibility. 7075 in the T6 temper is more susceptible, especially in the short-transverse grain direction; T73 greatly reduces this risk.
Surface protection: 6061 anodizes to a protective, often decorative coating. 7075 anodizes but the coating is less protective, so chromate conversion coating plus primer or paint is commonly applied.

Machining and Fabrication of 6061 vs 7075 Aluminum Alloys
Workability is the other decisive difference.
Machining: 6061 machines more easily because of its lower hardness; 7075 machines well too but needs appropriate tooling, speeds, and feeds, and causes more tool wear.
Forming: 6061's lower strength makes it easier to form, bend, and draw. 7075 is less formable and springs back more.
Joining - welding: 6061 is weldable with proper filler metal (commonly 4043 or 5356); post-weld heat treatment and aging may be required to recover the original T temper. 7075 is generally considered not weldable by fusion welding because it is prone to cracking in the heat-affected zone; mechanical fastening or adhesive bonding is used for 7075 joints. (This is a process limitation, not an application exclusion.)
Other joining: both can be joined by brazing, soldering, or adhesives where fusion welding is unsuitable.
Surface Treatment of 6061 and 7075 Aluminum Alloys
| Finish | 6061 | 7075 |
|---|---|---|
| Mill finish | Common | Common |
| Anodizing | Good, protective and decorative | Possible, but coating less protective |
| Chromate conversion | Used | Frequently used as a paint base |
| Powder / paint | Used | Common for corrosion protection |
Weight and Volume Calculation for 6061 and 7075 Aluminum Alloys
Weight is density multiplied by volume. For flat product, a quick rule is:
weight (kg/m²) = density (g/cm³) × thickness (mm)
6061: 2.70 kg per mm of thickness per square meter.
7075: 2.81 kg per mm of thickness per square meter.
For round bar, weight (kg/m) = density × π × r². A Ø25 mm 6061 bar weighs about 1.33 kg/m; the same Ø25 mm 7075 bar weighs about 1.38 kg/m - the ~4% density difference repeated at every section.
Applications of 6061 and 7075 Aluminum Alloy
The two grades overlap as structural alloys - both appear in bicycle parts, aerospace components, and building construction - but they are specified for different reasons.
6061 applications:
Structural frameworks, frames, and jigs where weldability matters.
Truck, trailer, and marine structures exposed to weather.
Piping, tanks, and vessels where formability and corrosion resistance help.
Bicycle frames and components built by welding or brazing.
Architectural and decorative sections, railings, and trims.
General machining blanks and fixtures.
7075 applications:
Highly stressed airframe parts - spars, fittings, wing skins, and brackets.
Performance and climbing hardware where peak strength-to-weight is required.
Molds, die plates, and precision tooling.
High-stress bicycle and motorsport components.
Defense and ordnance components where strength dominates.
6061 vs 7075 Aluminum Alloys: Side-by-Side Data Comparison
| Criterion | 6061-T6 | 7075-T6/T651 |
|---|---|---|
| Series / family | 6xxx (Al-Mg-Si) | 7xxx (Al-Zn-Mg-Cu) |
| Tensile strength | 310 MPa | 572 MPa |
| Yield strength | 276 MPa | 503 MPa |
| Density | 2.70 g/cm³ | 2.81 g/cm³ |
| Corrosion resistance | Good (general & marine) | Lower; SCC care needed |
| Weldability | Weldable (4043/5356) | Not fusion-weldable |
| Machinability | Good | Good, more tool wear |
| Formability | Good | Limited |
| Relative cost index | Lower (indicative) | Higher (indicative) |
Cost index is indicative and market-dependent; GNEE prices are benchmarked to SMM (Shanghai Metals Market).
Forms and Typical Dimensions of 6061 and 7075 Aluminum Alloys
6061 forms: plate, sheet, bar, rod, tube, pipe, extruded profile, and angle - the widest form range of the two.
7075 forms: plate, bar, and rod are the most common; extrusions and forgings are available; tube and pipe are less common.
Typical plate thickness: 1.0–150 mm (form-dependent).
Typical bar diameter: 6–300 mm for rolled and drawn product.
Exact available sizes depend on mill schedule; confirm the required form and dimensions with the supplier.
Quality Control and Mill Certificate for 6061 and 7075 Aluminum Alloys
Every order ships with an EN 10204 3.1 mill test certificate; 3.2 and third-party inspection can be arranged.
Mechanical properties are verified per the governing standard (e.g., ASTM B209 for flat product, ASTM B211/B221 for bar and extrusion).
For 7075 aerospace-grade plate, ultrasonic testing per ASTM B594 is commonly specified to check for internal defects.
Dimensional tolerances are inspected against the ordered standard and thickness range.

Export and Compliance Notes for 7075 Aluminum
Export control - read before ordering 7075. 7075 aluminum is listed on China's dual-use export-control catalogue. Control applies only when both of these are true: (1) ultimate tensile strength is ≥ 460 MPa at 20℃, and (2) the product is a cylindrical solid bar or a tube / pipe with outer diameter > 75 mm. When both are met, the item is subject to export licensing control and cannot be exported - GNEE does not supply these forms for export. Forms that fail either condition (plate, sheet, coil, strip, foil, tubes ≤ 75 mm OD, profiles, extrusions, forgings) are not in the controlled category and are exportable after standard first-round screening. 6061 is not on the controlled list. GNEE does not export to any party or destination prohibited under applicable export-control and international sanctions laws.
7075 aluminum forms that cannot be exported (dual-use control)
| Product form | Typical tempers | UTS @20℃ (MPa) | Control status |
|---|---|---|---|
| 7075 solid round bar (cylindrical solid bar) | T6 / T651, T73 / T7351, T76 / T7651 | 485 – 570 (all ≥ 460) | Cannot be exported |
| 7075 tube / pipe, outer diameter > 75 mm | T6 / T651, T73 / T7351, T76 / T7651 | 485 – 570 (all ≥ 460) | Cannot be exported |
Every common 7075 temper listed reaches UTS ≥ 460 MPa, so all 7075 solid bars and all 7075 tubes/pipes above 75 mm OD are controlled and cannot be exported.
7075 and 6061 aluminum forms that are exportable
| Product form | Alloy | UTS @20℃ (MPa) | Control status |
|---|---|---|---|
| Plate / sheet / coil / strip / foil (flat-rolled) | 7075 | 485 – 570 | Exportable after first-round screening |
| Tube / pipe, outer diameter ≤ 75 mm | 7075 | 485 – 570 | Exportable (not a controlled form) |
| Profile / extrusion / forging | 7075 | 485 – 570 | Exportable (not a controlled form) |
| All forms (plate, bar, tube, profile, etc.) | 6061 | ≤ 310 | Not controlled - exportable |
UTS values are drawn from GB/T, ASTM, and AMS standards (typical ranges). The 460 MPa threshold and the >75 mm tube / solid-bar form condition are the control triggers per China's dual-use list. Confirm the exact form and temper with GNEE before ordering.
Export Packaging of 6061 and 7075 Aluminum Alloys
Seaworthy export packing on fumigated wooden pallets or in wooden cases.
Interleaving with moisture-proof paper and plastic film to protect surfaces.
Steel strapping and edge protectors to secure and prevent transit damage.
Custom crating available for long bars and precision-machined parts.
Comparing 6061 and 7075 for a specific part? Tell GNEE the alloy, temper, form, dimensions, quantity, and destination, and we will confirm stock, lead time, and the applicable standard, then return a quotation with full specifications and the mill test certificate.
About GNEE
GNEE has supplied aluminum mill products across the 1xxx–8xxx range to customers in 100+ countries and regions since 2008.
Both 6xxx structural grades such as 6061 and 7xxx high-strength grades such as 7075 are stocked in common tempers and sizes for fast response.
Trial and volume orders are both accepted; minimum order quantity is flexible.
Material ships with EN 10204 3.1 MTC; 3.2 and third-party inspection can be arranged.
A technical team helps buyers match alloy, temper, and standard to the actual working condition, including export screening for controlled grades.
FAQ about 6061 vs 7075 Aluminum
Q: Which is stronger, 6061 or 7075 aluminum?
A: 7075. In the T6 condition, 7075-T6/T651 has a minimum tensile strength of 572 MPa (83 ksi) against 6061-T6 at 310 MPa (45 ksi) - about 1.8 times higher - and roughly 1.6 times the shear strength. 7075 also has a higher yield strength (503 MPa vs 276 MPa).
Q: Can 7075 be welded like 6061?
A: No. 6061 is weldable with proper filler selection (commonly 4043 or 5356); post-weld heat treatment and aging may be needed to recover the original T temper. 7075 is generally considered not weldable by fusion welding because it is prone to cracking in the heat-affected zone; mechanical fastening or adhesive bonding is used instead. Both can be joined by brazing, soldering, or adhesives.
Q: Which alloy is easier to machine?
A: 6061. Its lower hardness allows easier machining than 7075, which requires appropriate tooling and speeds because of its higher hardness. Both machine well with correct parameters; 7075's higher strength causes more tool wear.
Q: Is 7075 used only in aerospace?
A: No. 7075 also appears in climbing and performance hardware, bicycle components, molds and die plates, and other industrial tooling wherever maximum strength is needed, but aerospace is its most prominent market.
Q: Which alloy resists corrosion better, 6061 or 7075?
A: 6061. As a 6xxx alloy it shows good general and marine corrosion resistance and anodizes to a protective coating. 7075 (7xxx, high zinc and copper) has lower general corrosion resistance and is more susceptible to stress-corrosion cracking, especially in the short-transverse direction; the T73 temper improves this and protective finishing is commonly applied.
Q: Can 6061 and 7075 be used for the same parts?
A: They overlap as structural grades - both appear in bike parts, aerospace components, and building construction - but suit different priorities. 6061 is typical where corrosion resistance, weldability, and formability matter; 7075 is typical where the highest strength is required and some workability can be traded off. Whether one can stand in for the other on a given design must be confirmed against the load, environment, and joining method.