Overview of ASTM B209 7075-T651 Aluminum Plate Specifications

Dec 31, 2025

7075-T651 product forms and export availability

The PRC control list applies a two-condition trigger: an item is controlled only when both (a) its room-temperature ultimate tensile strength reaches ≥ 460 MPa (67 ksi) and (b) its shape is a tube with outside diameter > 75 mm or a cylindrical solid bar. The table below applies that test to each 7075 product form. GNEE flags all 7075 as a restricted export product, but only the forms marked "Not available" are genuinely barred by the list itself. In the T651 temper the typical tensile is ~572 MPa (83 ksi) - it meets the 460 MPa strength leg - yet 7075-T651 plate is flat-rolled and not a controlled form, so GNEE screens every order and supplies plate after a passed licence check.

 

Product form Typical temper Typical UTS (MPa / ksi) Meets control trigger? Export status
Plate / sheet / foil (flat-rolled, all thickness) O, T6/T651, T73/T7351, T76/T7651 275 – 572 MPa (40 – 83 ksi) No - flat-rolled is not a controlled form Restricted - supplied only after export-licence screening and end-use certification
Tube / pipe, outside diameter ≤ 75 mm T6, T73 485 – 540 MPa (70 – 78 ksi) No - OD ≤ 75 mm Restricted - licence screening required
Tube / pipe, outside diameter > 75 mm T651, T7351 up to ~572 MPa (83 ksi) Yes when UTS ≥ 460 MPa Not available for export
Cylindrical solid bar / rod T651, T7351 up to ~572 MPa (83 ksi) Yes when UTS ≥ 460 MPa Not available for export
Extruded profiles / shapes T651, T7351 480 – 560 MPa (70 – 81 ksi) No - not a controlled form Restricted - licence screening required
Forgings / die forgings T73, T7651 460 – 540 MPa (67 – 78 ksi) No - not a controlled form Restricted - licence screening required

UTS ranges are indicative and vary with temper and product thickness; values above 460 MPa (67 ksi) occur in the T6/T651/T73 heat-treated tempers. For the two controlled forms, GNEE does not supply 7075 to any destination. For the other 7075 forms, GNEE supplies only after a passed compliance screening; buyers who cannot license can evaluate 5083-H116, 6082-T6 or 6061-T6.

 

7075-T651 is the peak-strength, stress-relieved condition of the 7075 aluminum-zinc-magnesium-copper (7xxx-series) wrought alloy - the highest-strength aluminum plate in routine commercial use. GNEE supplies 7075-T651 aluminum plate rolled to ASTM B209, EN 485, GB/T 3880 and JIS H4000, the standard choice where maximum strength-to-weight ratio is the design driver. 

 

1. Which standards apply to 7075-T651 aluminum alloy?

7075-T651 is the peak-aged, stress-relieved temper of a heat-treatable Al-Zn-Mg-Cu (7xxx-series) wrought aluminum alloy covered by one family of rolled-product standards: ASTM B209, EN 573-3 / EN 485, GB/T 3190 / GB/T 3880, JIS H4000 and ISO 209-1. The "T651" designation is defined within these same standards as solution heat treated, stretched, then artificially aged. 7075 is widely used because, in T651, it delivers the highest strength of any commercially available aluminum plate - about 572 MPa (83 ksi) tensile - at a fraction of steel's weight for aerospace and structural duty.

Send an Inquiry Now

2. 7075-T651 Aluminum Equivalent Designations

Standard System Designation Notes
AA (Aluminum Association) 7075-T651 Peak-aged, stretched plate temper of 7075; base four-digit 7075
UNS A97075 Unified Numbering System, all tempers incl. T651
EN EN AW-7075 / AlZn5.5MgCu European designation; T651 = solution + stretch + age
DIN AlZnMgCu1.5 (3.4365) German equivalent; often quoted as 3.4365-T651
JIS A7075P-T651 (JIS H4000) Japanese plate/sheet designation, peak-aged stretched
GB (China) 7A09-T651 (GB/T 3190 / GB/T 3880) Closest national grade; T651 peak-aged; verify per order
ISO AlZn5.5MgCu / ISO 209-1 International composition designation

Equivalent designations describe the same base alloy; the "T651" suffix is carried through each system as the solution heat treated, stretched and artificially aged condition. The Chinese 7A09 is the long-standing national grade most often quoted as the GB equivalent of 7075 and is confirmed per mill certificate.

 

7075-T651 aluminum alloy

 

3. Chemical Composition of 7075-T651 Aluminum Plate (wt %) - per ASTM B209

The chemical limits below apply to the 7075 alloy family and therefore to the T651 temper; heat treatment changes the temper, not the composition. Values are composition limits per ASTM B209; actual mill certificate values vary within range.

Element Symbol Min (%) Max (%) Role / Function
Zinc Zn 5.10 6.10 Primary strengthening element; forms MgZn₂ (η-phase) precipitates
Magnesium Mg 2.10 2.90 With Zn drives precipitation hardening; raises strength
Copper Cu 1.20 2.00 Improves peak strength and machinability; aids SCC resistance at low levels
Chromium Cr 0.18 0.28 Controls grain structure and improves stress-corrosion resistance
Manganese Mn - 0.30 Trace grain refiner; limited to protect corrosion behaviour
Silicon Si - 0.40 Impurity; kept low to protect toughness and corrosion
Iron Fe - 0.50 Impurity; forms intermetallics, limited for ductility
Titanium Ti - 0.20 Grain refiner
Zirconium Zr - 0.05 Trace grain refiner when specified in lieu of Cr
Others (each / total) - - 0.05 / 0.15 Individual and total impurity limits
Aluminum Al Remainder Remainder Base metal

 

4. Mechanical Properties of 7075 Aluminum Plate by Temper (with T651 as the anchor)

The T651 temper is the peak-strength, stress-relieved condition this article centres on. The table lists ASTM B209 typical values; the T651 row is highlighted as the focus, with ksi equivalents in parentheses. T651's strength is the highest in the family - full precipitation hardening plus a stretch for flatness and stability.

7075-T651 - the anchor condition. Typical properties: Tensile strength 572 MPa (83 ksi), Yield strength 0.2% 503 MPa (73 ksi), Elongation ~11%, Hardness ~150 HB, Shear ~331 MPa (48 ksi). This is the highest-strength 7075 plate GNEE supplies, used where maximum load capacity per kilogram is the design driver.

Temper UTS (MPa) Yield 0.2% (MPa) Elongation (%) Hardness (HB) Shear (MPa)
7075-O 228 (33) 103 (15) 17 ~60 ~152 (22)
7075-T651 572 (83) 503 (73) 11 ~150 ~331 (48)
7075-T73 / T7351 524 (76) 455 (66) 11 ~140 ~296 (43)
7075-T76 / T7651 552 (80) 483 (70) 11 ~145 ~314 (45)

UTS and yield are ASTM B209 typical values for plate; elongation and hardness are indicative. The T651 temper achieves the top tensile/yield of the family at the cost of reduced formability and lower SCC resistance than the overaged T73/T76 tempers.

 

5. Physical Properties of 7075-T651 Aluminum Plate (Typical)

Physical properties are essentially independent of temper, so the values below apply to 7075-T651 as supplied. Sources: ASM Handbook and ASTM reference data.

Property Value Unit
Density 2.81 g/cm³ (0.1015 lb/in³)
Melting range 477 – 635 °C (890 – 1175 °F)
Elastic modulus 71.7 GPa (10.4 × 10³ ksi)
Shear modulus 26.9 GPa (3.9 × 10³ ksi)
Poisson's ratio 0.33 dimensionless
Electrical conductivity 33 % IACS (typical, T6/T651)

 

6. Heat Treatment & Temper Guide for 7075 Aluminum Plate

7075-T651 is produced by solution heat treatment, a controlled stretch to relieve residual stress, and artificial aging to peak hardness. The softer tempers are either fully annealed (O) or overaged (T73/T76) for corrosion resistance. Exact soak times vary with thickness and are [To be confirmed] per furnace schedule; the temperatures below are the standard windows.

Temper Process Characteristics Typical Use
O Annealed ~415 °C (775 °F), furnace-cooled Softest, most formable, lowest strength Forming stock before heat treatment
T651 Solution 465 °C ±10 °C (870 °F); stretched 1.5–3%; Age 120 °C (250 °F) × 24 h Peak strength + good dimensional stability Highest-strength aerospace and structural plate
T73 / T7351 Solution 465 °C; overaged 107 °C × 8 h + 177 °C × 8 h (two-step) Slightly lower strength, much better SCC resistance Thick sections, sustained-tension service
T76 / T7651 Solution 465 °C; overaged (single-step, less than T73) Balanced strength and exfoliation resistance Skins and plate needing corrosion margin

Solution temperature is indicative at ~465 °C (870 °F) and aging near 120 °C (250 °F) for T651; exact cycles are [To be confirmed] and depend on section thickness. The stretch in T651 is what distinguishes it from plain T6 and gives the plate its low warp after machining.

 

7. The Product Specification of 7075-T651 Aluminum Plate

Parameter Details
Alloy & temper 7075-T651 (solution heat treated, stretched, aged)
Thickness 4 – 150 mm (0.16 – 6 in), per ASTM B209
Width up to 2500 mm (98 in)
Length up to 12000 mm (39 ft)
Standards ASTM B209, EN 485, GB/T 3880, JIS H4000
Package Export seaworthy: PE film + interleaving paper, edge protectors, wooden pallet/case with moisture barrier
Cladding option Alclad 7075 (7072 cladding) available for corrosion-critical service

 

7075 T651 aluminum plate ASTMB209 3010002000mm

 

8. Corrosion Resistance of 7075-T651 Aluminum Plate

Atmospheric: 7075-T651 is among the least corrosion-resistant high-strength aluminums because of its high zinc and copper content; in untreated exposure it pits and exfoliates more readily than 2xxx or 6xxx plate.

Marine: Poor in bare form. For salt exposure, 7075 is normally supplied as Alclad (7072 cladding) or painted; the cladding sacrifices itself to protect the core. T73/T76 tempers add exfoliation resistance.

Galvanic: As a copper- and zinc-bearing alloy it is cathodic to most other aluminum and to steel; dissimilar-metal contact should be insulated to avoid galvanic attack of the adjacent metal.

Stress-corrosion cracking (SCC): The T651 temper is the most SCC-prone condition of 7075 under sustained tensile stress, especially in thick sections and short-transverse grain direction. For such service, T73/T7351 or T76 is specified instead.

Recommended surface treatments: Alclad cladding, chemical conversion coating (e.g. Alodine), anodizing (thin Type II, usually followed by sealant/paint), primer/paint systems, or PVDF coating - applied as a system, not a single finish.

 

9. Fabrication and Processing of 7075-T651 Aluminum Plate

9.1 Welding of 7075-T651 aluminum plate

Fusion welding is generally not recommended for 7075 in any temper: the alloy is hot-crack sensitive and the heat-affected zone loses precipitation strength, dropping toward the annealed level of about 275 MPa (40 ksi). Resistance welding (spot, seam) is acceptable for assembly; where fusion joining is unavoidable, filler 5356 or 4043 is used for non-structural joints. Riveting, bolting or adhesive bonding remain the norm for load-bearing 7075-T651 structures.

9.2 Machinability of 7075-T651 aluminum plate

7075-T651 is rated A on the AA machinability scale - one of the best machining aluminum alloys. Its high strength and fine, stable grain take high speeds and feeds with an excellent finish and long tool life. Carbide tooling and copious coolant are standard; the low residual stress from the T651 stretch keeps parts stable after material removal.

9.3 Formability of 7075-T651 aluminum plate

Formability is the weak point of the T651 temper: with elongation near 11% and peak strength, 7075-T651 takes only large bend radii (typically 3–4 × thickness or more) and is not for deep drawing or tight cold forming. Where forming is required, the part is rough-formed in O temper and then heat treated to T651, or a more formable grade such as 6061-T6 / 6082-T6 is selected.

9.4 Surface Finishes for 7075-T651 aluminum plate

Finish Description Application
Mill finish As-rolled, untreated surface Structural and machined parts prior to coating
Alclad (7072) Pure-aluminum cladding metallurgically bonded to both faces Corrosion-critical aerospace and marine plate
Chemical conversion (Alodine) Chromate-free phosphate coating Paint base / corrosion primer for assemblies
Anodized (Type II) Thin oxide layer, 5–25 µm Appearance and mild wear (usually painted after)
Powder / PVDF coat Polymer or fluoropolymer film Exterior and marine-exposed surfaces

 

Get Project Quotation

 

10. Applications of 7075-T651 Aluminum Plate

Aerospace - primary structures: wing skins, fuselage frames and spar caps are cut from 7075-T651 plate for its ~572 MPa (83 ksi) tensile - the highest strength-to-weight of any aluminum plate, cutting airframe mass.

Aerospace - fittings & landing gear brackets: high-load brackets and gear components use 7075-T651 for its peak yield of 503 MPa (73 ksi) where every kilogram saved matters and the part is machined from solid.

Defense - armor & ordnance: military vehicle armor plate and missile structural components use 7075-T651; its strength lets thin, light plates meet ballistic and structural targets.

Tooling & mold bases: plastic injection mold bases, jigs and fixtures use 7075-T651 for its AA-rating-A machinability and dimensional stability; the stretched plate stays flat after heavy material removal.

Sporting goods: climbing carabiners, bicycle frames and rifle receivers use 7075-T651 for strength at low weight where a small, highly loaded part must not fail.

Industrial machinery - high-strength frames: machine bases and robotic arms use 7075-T651 where stiffness and low mass beat cost; it machines cleanly to tight tolerances.

Automotive (performance): racing suspension arms and chassis brackets use 7075-T651; its yield lets engineers down-gauge and cut unsprung mass.

Electronics - precision bodies: camera and instrument chassis use 7075-T651 for rigidity at minimal thickness where a stiff, stable, lightweight frame is required (coated for corrosion).

Marine (Alclad only): where 7075's strength is mandated offshore, Alclad 7075 plate is used for high-stress fittings, with 7072 cladding providing the corrosion barrier.

Oil & gas - downhole tools: logging-tool bodies and sub-assemblies use 7075-T651 for strength-to-weight in confined bores (selected in T73 for sour-service SCC margin).

 

11. 7075-T651 vs 2024-T351 vs 6061-T651 vs 7050-T7451 Aluminum Plate: Key Differences

Because 7075-T651 is chosen for peak strength, the useful comparison is against other high-strength aerospace plate alloys. All four rows are representative commercial tempers, with quantified properties from ASTM/EN reference data.

Series Heat-treatable? UTS MPa Yield MPa Elongation % Relative cost (indicative) Primary use
7xxx (7075-T651) Yes 572 503 11 Higher (~1.6× 6061) Highest-strength aerospace & structural plate
2xxx (2024-T351) Yes 470 325 17 Medium (~1.3× 6061) Fatigue-critical skins, good damage tolerance
6xxx (6061-T651) Yes 310 276 12 Medium (1.0× baseline) General structural, weldable, lower cost
7xxx (7050-T7451) Yes 524 462 11 Higher (~1.7× 6061) Thick-section aerospace, high fracture toughness

Cost indices are indicative and benchmarked to SMM; actual spreads move with the zinc, copper and magnesium premiums. 7075-T651 leads on absolute strength but trails 2024-T351 on fatigue tolerance and 6061-T651 on weldability and cost; 7050-T7451 is the thick-section alternative with better toughness. Buyers who cannot meet 7075 licensing can evaluate 5083-H116, 6082-T6 or 6061-T6.

 

12. FAQ

What does the T651 temper mean for 7075 aluminum plate? T651 = solution heat treated, stretched 1.5–3% to relieve residual stress, then artificially aged to peak strength; it gives about 572 MPa (83 ksi) tensile and 503 MPa (73 ksi) yield with good stability after machining.

Can 7075-T651 aluminum plate be welded? Fusion welding is generally not recommended - hot-crack sensitive and the HAZ drops toward ~275 MPa (40 ksi). Resistance welding is fine; for unavoidable fusion joints use 5356/4043 fillers non-structurally; riveting/bonding remain common.

What is the maximum service temperature for 7075-T651 plate? About 120 °C (250 °F) sustained. Above that, strength falls, so 7075-T651 is not a high-temperature alloy; 2xxx grades are used where heat resistance is needed.

How does 7075-T651 differ from 7075-T73 plate? Same base alloy; T73 is two-step overaged for much better SCC resistance at a small strength cost (524/455 MPa vs 572/503 MPa). T651 for maximum strength, T73/T7351 for thick or sustained-tension service.

What sizes does GNEE supply in 7075-T651, and how is it packed? GNEE supplies 7075-T651 plate from 4 mm to 150 mm thick, up to 2500 mm wide and 12000 mm long, packed for export with PE film, interleaving paper, edge protectors and seaworthy wooden pallets/cases.

Is 7075-T651 aluminum plate subject to export control? Yes. 7075 is a controlled-grade alloy under the PRC dual-use regime; GNEE classifies 7075-T651 plate as a restricted export product requiring a licence and end-use certification. The T651 tensile (~572 MPa) meets the 460 MPa threshold but the plate is flat-rolled, so GNEE screens and supplies after a passed check; buyers who cannot license can evaluate 5083-H116, 6082-T6 or 6061-T6.

 

About GNEE

GNEE is an aluminum manufacturer established in 2008, exporting to 100+ countries and regions, with a technical team that selects tempers against your strength, corrosion and machining route.

For 7075-T651 plate, GNEE holds common thicknesses in stock and supplies both the peak-aged T651 temper and the overaged T73/T76 tempers where SCC margin or thick-section toughness is required.

MOQ is flexible - both small trial orders and large-volume orders are accepted, and larger contracts are welcome; lead time runs about 15–30 days.

Every 7075 order is screened against the current PRC export-control list before a quote is released; supply requires an export licence and end-user / end-use certification. Buyers who cannot meet licensing can evaluate 5083-H116, 6082-T6 or 6061-T6.

Documentation with every export shipment. EN 10204 3.1 mill test certificate is standard; 3.2 with third-party witnessing (SGS, BV, TÜV) is available on request. Quotes are benchmarked to SMM with a reply within 24 hours.

7075 t651 aluminum plate EN 485-2-2013 90x1250x2500