7075 sheet and plate is the high-strength copper-bearing aluminium alloy that most engineers reach for when a part must be light and highly loaded at the same time. Its strength approaches that of some steels at about one third of the weight, but it is also the alloy family in which temper selection carries the greatest consequence, because the strongest tempers are the least resistant to stress-corrosion cracking. Understanding what T6, T651 and T7351 actually mean is therefore a design decision, not a purchasing detail.
Temper Designations Decoded
The designations follow the American National Standard temper system, ANSI H35.1, and are the same ones carried into ASTM B209/B209M. T6 means solution heat treated and then artificially aged to peak strength. T651 adds a stress-relief step: after quenching, the product is stretched by a controlled amount to introduce a permanent set, which relieves internal stress and greatly reduces distortion when a part is machined out of thick plate. T7351 is the same processing route with a deliberately overaged condition, trading a modest amount of strength for much better resistance to stress-corrosion cracking and exfoliation. Heavy plate is almost always ordered in T651 or T7351, because T6 plate is not stretch relieved and will move during machining.
Export Control Notice - These Grades Cannot Be Exported
7075 aluminum - including forged 7075-T6 - falls within these categories and is not available for export.
High-strength aluminum alloys of this class are listed under the export control regulations of the People's Republic of China for dual-use items and technologies. Shipping them out of China requires an export licence issued by the competent Chinese authorities. In practice a licence is not obtained for ordinary commercial orders in these categories, so GNEE does not export them.
GNEE does not export to any party or destination prohibited under applicable export control and international sanctions laws.
Control status technically turns on six variables: alloy grade, temper, product form, dimensions, quantity and intended end-use. Whatever the combination, none of the grades in the table below are available for export from GNEE.
Aluminum grades affected by these controls
| Alloy grade | Common temper(s) | Tensile strength (MPa) - reference |
|---|---|---|
| 7075 | T6 / T651 | 540 – 570 |
| 7075 | T73 / T7351 | 485 – 500 |
| 7075 | T76 / T7651 | 500 – 515 |
| 7050 | T7451 / T6 | 475 – 620 |
| 2024 | T351 / T4 | 425 – 470 |
| 7A04 | T6 | ≥ 530 |
| 2014 | T6 | approx. 460 – 500 |
| 2017 | T4 | approx. 390 – 480 (some specifications may reach higher) |
| 2195 | - | approx. 572 |
| 7068 | - | approx. 623 |
| 7055 | - | approx. 654 |
| 7150 | - | approx. 643 |
Strength values in this table are indicative reference ranges used for control classification. They are not specification minimums. The governing limits for any enquiry come from the applicable standard or your drawing.
What we can quote instead
We cannot accept export enquiries for the grades listed above. If strength is the reason you are looking at them, send us the load case, the service environment and the fabrication method, and we will quote a non-controlled substitute - usually from the 5xxx or 6xxx series - with properties that fit the job and no export restriction attached.
Composition Limits
| Element | Limit (mass %) | Function |
|---|---|---|
| Zn | 5.1-6.1 | Principal strengthening addition |
| Mg | 2.1-2.9 | Forms the strengthening precipitate with zinc |
| Cu | 1.2-2.0 | Raises strength, reduces corrosion resistance |
| Cr | 0.18-0.28 | Grain structure, improves stress-corrosion behaviour |
| Fe | 0.50 max | Impurity, controlled for toughness |
| Si | 0.40 max | Impurity |
| Mn | 0.30 max | Impurity |
| Ti | 0.20 max | Grain refiner |
| Others | Each 0.05 max, total 0.15 max | - |
| Al | Remainder | Balance |
Strength and Physical Properties
| Property, room temperature | 7075-T6 / T651 | 7075-T7351 |
|---|---|---|
| Typical tensile strength | approx. 572 MPa (83 ksi) | approx. 505 MPa (73 ksi) |
| Typical 0.2 % yield strength | approx. 503 MPa (73 ksi) | approx. 435 MPa (63 ksi) |
| Typical elongation, 2 in. | approx. 11 % | approx. 10 % |
| Density | 2.81 g/cm3 | 2.81 g/cm3 |
| Elastic modulus | approx. 71.7 GPa | approx. 71.7 GPa |
These are typical published values for the tempers. Minimum guaranteed values depend on product form, thickness and direction, and are tabulated in ASTM B209/B209M; a certificate of conformance should be read against those minima rather than against typical figures. Heat treatment itself is controlled to aerospace practice, for which the AMS heat treatment specification for aluminium alloy raw materials is the usual contractual reference.
Stress-Corrosion and Exfoliation Behaviour
7075 in the T6 temper is the classic example of a high-strength alloy that is not suitable for sustained tensile stress in a corrosive environment, especially when the stress acts across the short-transverse direction of a thick section. Overaging to T73, and the associated T7351 stretched product, was developed specifically to remove that limitation at the cost of roughly ten per cent of the tensile strength. The tests that decide acceptance are ASTM G47 for susceptibility to stress-corrosion cracking, ASTM G34, the exfoliation corrosion test known as EXCO, and ASTM G44 for alternate immersion exposure. In production, temper is also verified non-destructively by electrical conductivity measurement using the eddy-current method of ASTM E1004, because the overaged T73 condition sits at a distinctly higher conductivity than the T6 condition. That conductivity check is a useful incoming-inspection tool for any shop that machines 7075.
Machining, Forming and Finishing
The alloy machines well and is a mainstay of high-speed machining of structural parts, with carbide tooling, generous coolant and attention to chip evacuation. Distortion control matters more than cutting parameters: stretch-relieved T651 or T7351 plate, symmetrical material removal and intermediate stress-relief where large amounts of stock are removed. 7075 is not normally fusion welded; the copper content makes the alloy prone to cracking and the heat-affected zone loses strength, so parts are joined mechanically or, where welding is unavoidable, an entirely different alloy family is selected. Forming in the aged tempers is limited to gentle radii, and parts that must be bent sharply are usually formed in a softer condition and heat treated afterwards. Hard anodic coatings to MIL-A-8625 Type III are routinely applied and give excellent wear resistance; a chromate-free conversion coating is used where corrosion protection without build-up is required.
Typical Applications
Applications include aircraft fittings, structural brackets and clips, actuation components, gears and shafts, tooling and fixture bodies, mould cavities, drone and unmanned-vehicle airframes, high-performance bicycle and motorcycle components, and any highly stressed machined part where weight saving has value. In all of these the temper decision follows from the stress state and the environment rather than from strength alone: parts loaded continuously in tension in a corrosive atmosphere should be specified in T7351 plate, while parts that are protected, loaded in compression or loaded only in the short term can use T6 or T651.
Frequently Asked Questions
Q: What is the difference between 7075-T6 and 7075-T651?
A: They have essentially the same strength. T651 product is stress relieved by stretching after quenching, which reduces internal stress and distortion during machining. Thick plate for precision parts is normally specified as T651.
Q: Why choose T7351 when it is weaker than T6?
A: Because T7351 is far more resistant to stress-corrosion cracking and exfoliation. In thick sections under sustained tensile stress in a corrosive environment, the overaged temper is the correct engineering choice despite losing roughly ten per cent of the tensile strength.
Q: Can 7075 be welded?
A: It is not normally fusion welded. The alloy is crack sensitive and the heat-affected zone is severely weakened. Mechanical fastening is preferred, or a different alloy family is selected for welded assemblies.
Q: How can I verify the temper of delivered plate?
A: By measuring electrical conductivity with the eddy-current method of ASTM E1004. The overaged T73 condition is clearly distinguishable from the T6 condition, and conductivity checks are widely used as a rapid incoming-inspection screen.
Q: What corrosion tests apply to 7075 tempers?
A: ASTM G47 for stress-corrosion cracking, ASTM G34 for exfoliation corrosion, and ASTM G44 for alternate immersion exposure are the standard methods referenced when the corrosion behaviour of the temper must be demonstrated.
Q: Which tempers are available as sheet as well as plate?
A: Thin sheet is commonly supplied in T6, while plate from about 0.250 in (6.35 mm) upwards is stocked mainly in the stretched tempers T651 and T7351, because those are the forms in which dimensional stability after machining is required.