What Corrugated Aluminium Metal Is
Corrugated, or profiled, aluminium is produced by passing flat aluminium coil through a series of matched rolls that progressively bend the strip into a repeating section: sinusoidal, trapezoidal, and standing-seam are the common families. The ribs do not increase the strength of the metal itself; they increase its stiffness by moving material away from the neutral axis, which is why a 0.5 mm profiled sheet can span a distance that a flat sheet of the same gauge cannot.
The product is used as building cladding and roofing, as jacketing over pipe and duct insulation, as lining for cooling towers and agricultural buildings, and as corrugated cores in heat exchangers and solar air collectors.
Why 1050, 1060 and 1100
All three grades are commercially pure aluminium with different guaranteed minimum purity. Their shared advantages are high thermal and electrical conductivity, excellent corrosion resistance from the natural oxide film, good workability and low cost relative to alloyed sheet.
| Grade | Aluminium (min) | Other controlled elements | Density | Typical use |
|---|---|---|---|---|
| 1050 | 99.5% | Fe up to 0.40, Si up to 0.25 | 2.705 g/cm3 | General purpose profiled sheet, reflectors, flashings |
| 1060 | 99.6% | Fe up to 0.35, Si up to 0.25 | 2.705 g/cm3 | Insulation jacketing, decorative profiles |
| 1100 | 99.0% | Cu 0.05-0.20 | 2.710 g/cm3 | Higher-strength profiles, chemical equipment, heat exchangers |
Physical values shared by these grades: melting range of about 643 to 658 Celsius depending on purity, thermal conductivity in the region of 220 to 235 W/(m.K) for the pure grades, and an electrical conductivity around 59 to 61% IACS. Mechanical strength is modest, which is why the profile rather than the alloy carries the structural duty.
Profiles, Tempers and Gauge
Temper: H14, H16, H18 and H24 are the usual delivery tempers; H18 is used where the finished panel must be stiff and self-supporting.
Gauge: profiled aluminium is normally formed from 0.3 mm to 1.5 mm coil, with 0.5 mm to 1.0 mm dominant in construction.
Profiles: pitch and depth are set by the roll former; trapezoidal sections are standard for walls and roofs, sinusoidal sections for cheaper enclosures and jacketing.
Cover width: determined by the development of the profile, not by the coil width, and must be quoted together with the pitch.
Because the profile is formed from a coil of fixed width, the coil width decides the number of ribs and hence the cover width. Ordering to the wrong coil width produces a profile that cannot be lapped correctly with the rest of the building.
Applications in Detail
Building envelope
Corrugated aluminium is used for walls, roofs, canopies and agricultural buildings because it is light, does not rust in the way galvanised steel can, and reflects a large part of solar radiation. It is fixed through the crest of the profile with sealing washers.
Insulation jacketing
Thin profiled aluminium protects mineral wool, foam and pipe insulation from weather and mechanical damage on tanks, vessels and long pipe runs. Here the grade is often 1060 or 1100 for its combination of formability and corrosion resistance.
Heat transfer and reflectors
Because the 1xxx grades conduct heat efficiently, corrugated aluminium is used as fin stock, heat-exchanger cores and solar collector absorbers. Lamp reflectors and light fittings use 1050 or 1100 with a polished or anodised finish.
Other uses
Chemical process equipment cladding, food industry enclosures, cable trays, temporary structures, cable sheathing, pyrotechnic applications and architectural flashings all consume corrugated or profiled 1xxx aluminium.
Installation and Fabrication Points
Isolate aluminium from steel and, above all, from copper and copper alloys; in the presence of moisture a galvanic couple will corrode the aluminium.
Allow for thermal movement. Aluminium expands about twice as much as steel for the same temperature rise, so fixings should be positioned so the sheet can slide.
Cut with a fine-tooth blade or shear, and remove swarf immediately; embedded particles are the starting point for staining.
Use sealant compatible with aluminium, and avoid acidic silicone products that can attack the surface.
Store coils and sheets dry, off the ground and clear of condensation; white rust from trapped moisture is difficult to reverse.
Common Misconceptions
1100 is stronger than 1060, therefore always better. The copper addition raises strength slightly but lowers purity and slightly reduces conductivity; the right grade depends on the duty.
Corrugated aluminium is a structural material. It is a cladding and enclosure material. Design loads must be checked against the profile's span capability.
Purity and corrosion resistance are the same thing. Atmosphere, contact metals and surface treatment matter as much as the alloy.
Any roll former can produce any profile from any coil. Profile development depends on coil width and gauge; the tooling must match both.
FAQ
Q: What is the difference between 1050, 1060 and 1100 aluminium?
Their minimum aluminium content is 99.5%, 99.6% and 99.0% respectively; 1100 also contains 0.05 to 0.20% copper, which raises strength slightly.
Q: What is 1050 aluminium used for?
Chemical process plant equipment, pyrotechnic powder, lamp reflectors, food industry containers, cable sheathing and architectural flashings.
Q: What is 1100 aluminium used for?
Applications that need a little more strength than 1050 while retaining good formability, such as chemical equipment, food handling equipment, decorative items and heat exchangers.
Q: What is the difference between 1100 and 5052 aluminium?
1100 is a soft, low-strength commercially pure grade chosen for ductility; 5052 is an aluminium-magnesium alloy with much higher tensile and fatigue strength.
Q: Can corrugated aluminium be used outdoors?
Yes. It performs well in most atmospheres provided it is not in direct wet contact with copper or steel and the cut edges are protected where appearance matters.
Q: Which temper should be specified for roofing profiles?
H14 or H16 for profiles that must be formed without cracking, and H18 where maximum stiffness of the finished panel is required.